#548
Alloy
Thank you for using UNITED'S alloys.
UNITED’S
548 ALLOY may be used for 10K - 18K casting, or hand-made (rolling),
which produces a pink / red finished color.
You should obtain excellent results by following a few simple
instructions.
MELTING
| Melt
Temperature for 10 & 14K Alloyed Grain |
990° - 1010° C |
1814° - 1850° F |
| Melt
Temperature for 18K Alloyed Grain |
1010° C |
1850° F |
| Melt
Temperature for Alloying |
1050° - 1060° C |
1922° - 1940° F |
We do recommend pre-graining all alloy and fine gold before
casting to assure a uniform mixture.
FLASK TEMPERATURE
We
recommended a slightly higher temperature.
FLUXING
Boric Acid is the recommended flux. Use as little flux as
possible. Do not use carbon fluxes or any fluxes designed for
refining; i.e., soda ash, saltpeter, etc. Avoid flux in bottom pour
automatic casting units.
QUENCH TIME
For
10K & 14K quench 15 minutes.
For 18K quench A.S.A.P.
For hand-made (rolling), quench ingot immediately.
INVESTMENT REMOVAL
Most standard investment removers will
successfully remove the investment powder. Fluoric-based investment
removers are the best for removing the silicon oxide invisible
coating. Our Brite-Cast Investment Remover also works very well.
REMELTING
We recommend 50% rejuvenation for remelting.
NOTES
Melt temperature may vary with type of unit. This alloy is
designed for casting only.
TECHNICAL ASSISTANCE
Always available…
Call 1-800-999-3463 / 1-800-999-FINE
E-mail / doc@unitedpmr.com
Web-Site / www.unitedpmr.com |